Pilling is the formation of small balls of tangled fibre on a fabric surface. No laboratory test reproduces wear exactly, so standards create pills mechanically and then grade the result visually from 5 (no change) to 1 (severe pilling). The three common methods do this in different ways, and their grades are not interchangeable.
The three methods at a glance
Values below are from the editions we checked: EN ISO 12945-1:2000, EN ISO 12945-2:2000 and ASTM D3512-02. All three have been revised since, so check the current text before writing a procedure.
| ICI pilling box (ISO 12945-1) | Martindale (ISO 12945-2) | Random tumble (ASTM D3512) | |
|---|---|---|---|
| How pills form | Specimens mounted on tubes tumble in a cork-lined box | Specimen rubs against fabric or a wool abradant along a Lissajous path | Specimens tumble freely in a cork-lined chamber driven by an impeller, with air injection |
| Key apparatus | Box 235 mm inside, 3.2 mm cork lining, 60 ± 2 rpm; four polyurethane tubes 140 mm long | Holder 155 ± 1 g; with the extra disc 415 ± 2 g | 1.5 mm cork liners; 14–21 kPa air; about 25 mg of grey cotton fibre added |
| Specimens | Four 125 × 125 mm, sewn into tubes (two lengthwise, two widthwise) | Circular specimens and matching abradant; at least three pairs | Three 105 mm squares cut at 45° (bias), edges sealed |
| Test length | Number of revolutions agreed between the parties | Assessed at stages: 125, 500, 1 000, 2 000, 5 000, 7 000 rubs (woven and knitted) | 30 min unless otherwise agreed |
| Grade | 5 to 1, half grades allowed | 5 to 1 at each stage, half grades allowed | 5 to 1 against fabric or photographic standards |
ICI pilling box
The box method is simple and gentle. Its main open point is test length: ISO 12945-1 states that no single number of revolutions suits every fabric, so the number must be agreed and reported. A grade 4 after one revolution count and a grade 4 after another are different results. The cork lining must be inspected regularly and replaced when it is damaged or contaminated, because it is the rubbing surface. Specimens are conditioned for at least 16 h in the ISO 139 atmosphere before testing.
Martindale
The modified Martindale method rubs the specimen in a Lissajous figure, which changes direction continuously. ISO 12945-2 sets categories in its Annex A:
| Category | Abradant | Load | Assessment stages (rubs) |
|---|---|---|---|
| 1 Upholstery | Wool abradant fabric | 415 ± 2 g | 500 · 1 000 · 2 000 · 5 000 |
| 2 Woven (not upholstery) | Same fabric face to face, or wool | 415 ± 2 g | 125 · 500 · 1 000 · 2 000 · 5 000 · 7 000 |
| 3 Knitted (not upholstery) | Same fabric face to face, or wool | 155 ± 1 g | 125 · 500 · 1 000 · 2 000 · 5 000 · 7 000 |
For categories 2 and 3 the minimum is 2 000 rubs. Because the grade is recorded at each stage, a Martindale result shows how pilling develops and, for some fibres, how pills wear off again. The report must state the abradant, the load and the number of rubs at each stage. For more detail see our note on why two laboratories grade Martindale pilling differently.
Random tumble
In ASTM D3512, three bias-cut specimens tumble in a cork-lined chamber with a small amount of grey cotton fibre, which helps pills form with an appearance closer to worn garments. The cork liners matter: each face is discarded after 1 h of use, and the tester should be checked with an in-house reference fabric at least once a week when in constant use, and whenever a new shipment of liners arrives. ISO 12945-3 is the ISO random-tumble method; check it separately if your specification calls for it.
ASTM D3512 also gives a useful warning about precision: in its interlaboratory study, fabrics averaging 2.0 or below, or 4.0 or above, showed high agreement between laboratories, while fabrics between 2.0 and 4.0 showed low agreement. Mid-range grades are where disputes happen.
Which method should you use?
- Follow the buyer's specification. Brand and retailer standards name the method, the revolutions or rubs and the pass grade.
- Box suits routine quality control of knitwear and woven apparel when a revolution count is agreed.
- Martindale suits fabrics where the development of pilling over time matters, and upholstery.
- Random tumble is common where ASTM methods are specified.
Never convert a grade from one method to another. Report the method, edition, revolutions, rubs or running time, abradant, pre-treatment such as washing, and the number of observers.
Grading is the weak point
All three methods rely on visual assessment. ISO 12945-1 specifies the viewing set-up: light at 5° to 15° to the specimen plane, and a viewing distance of 30 to 50 cm. It also recommends more than one observer. Use the same viewing cabinet and the same photographic or fabric standards every time.
Frequently asked questions
Is a grade 4 on the box the same as a grade 4 on Martindale?
No. The mechanisms and test lengths differ, so the grades are not comparable.
How many revolutions should I run on the ICI box?
ISO 12945-1 leaves this to agreement between the parties. Use the number in your customer's specification and report it.
Why add cotton fibre in the random tumble test?
ASTM D3512 adds a small amount of short grey cotton fibre so that pills form with an appearance and structure closer to those produced in actual wear.