In a salt spray test, specimens sit in a closed cabinet while a salt solution is atomised into a fine fog that settles on them continuously. The two most cited methods are ISO 9227, with three variants, and ASTM B117. Both describe the cabinet and its conditions; the product specification decides the duration and the pass criteria.
The three ISO 9227 variants
- NSS (neutral salt spray): sodium chloride solution with a pH of 6.5 to 7.2.
- AASS (acetic acid salt spray): the same solution acidified with acetic acid to a pH of 3.1 to 3.3.
- CASS (copper-accelerated acetic acid salt spray): AASS solution with copper(II) chloride added at 0.26 g/l ± 0.02 g/l; it runs at a higher temperature.
Key conditions compared
ASTM values are from B117-03; ISO solution values are from ISO 9227:2022, while cabinet temperature, collection rate and specimen angle are from ISO 9227:1990, the edition whose text we could check for those clauses. Check the current editions before writing a procedure.
| Condition | ISO 9227 (NSS) | ASTM B117-03 |
|---|---|---|
| Salt solution | NaCl 50 g/l ± 5 g/l in the collected spray; water ≤ 20 µS/cm at 25 °C | 5 ± 1 parts by mass NaCl in 95 parts water |
| pH of collected solution | 6.5 to 7.2 at 25 °C ± 2 °C | 6.5 to 7.2, measured at 25 °C |
| Cabinet temperature | 35 °C ± 2 °C (NSS, AASS); 50 °C ± 2 °C (CASS) | 35 °C +1.1 / −1.7 °C in the exposure zone |
| Collection rate | 1 to 2 ml/h per 80 cm², averaged over at least 24 h | 1.0 to 2.0 mL/h per 80 cm²; at least two collectors |
| Specimen angle | About 20° from vertical, within 15° to 30° | 15° to 30° from vertical |
The numbers look almost identical, which is why many chambers are specified for both. The details still differ: ISO 9227 sets the concentration of the collected spray in g/l and adds AASS and CASS; B117 describes a single neutral fog. Report the standard you actually followed.
Checking that the cabinet is right
- Collection: fall-out, concentration and pH are measured from collectors placed in the specimen zone; ISO 9227:2022 specifies collectors with a collecting area of about 80 cm².
- Air supply: ISO 9227:2022 gives an atomising overpressure of 70 kPa to 170 kPa, typically 98 kPa ± 10 kPa; B117-03 suggests running the air saturator tower at about 46 °C to 49 °C for a 35 °C test.
- Corrosivity check: ISO 9227 verifies the cabinet with reference specimens of CR4 steel, 150 mm × 70 mm, with a surface roughness Ra of 0.8 µm ± 0.3 µm.
- Cabinet size: ISO 9227:2022 notes that cabinets smaller than 0.4 m³ are more sensitive to how they are loaded.
What the hours mean
ISO 9227:1990 lists recommended exposure periods from 2 h to 1 000 h; the actual period comes from the product specification or agreement. Neither standard turns hours into years. B117-03 states that prediction of performance in natural environments has seldom been correlated with salt spray results, and ISO 9227 describes the method as a check on the comparative quality of a coating, not a guide to long-term behaviour. Salt spray is best used to compare similar coatings and to monitor production consistency.
Where cyclic tests fit
A continuous fog never dries. Cyclic corrosion tests alternate salt exposure with drying and humidity phases, and many automotive specifications call for them. The TL-CCT-600 runs continuous neutral salt spray to ISO 9227 (NSS) and ASTM B117, and adds drying and high-humidity phases; the TL-CRH-1300 and TL-CRH-1100 are built for programmed cyclic corrosion profiles.
What the report should contain
Standard, edition and variant (NSS, AASS, CASS) · specimen description and preparation · cabinet temperature · collection rate, concentration and pH · specimen angle · test duration · evaluation method and result
Frequently asked questions
Is ISO 9227 NSS the same as ASTM B117?
The core conditions are very close, but they are separate standards with different wording and scope. Specify and report the one the customer asks for.
How many salt spray hours equal one year outdoors?
There is no conversion. Both standards warn against predicting service life from salt spray hours.
Why add acetic acid or copper chloride?
AASS and CASS are more aggressive variants used for specific coatings, such as decorative nickel-chromium plating; use them only when the specification calls for them.