The oxygen index (OI), often called the limiting oxygen index (LOI), is the minimum concentration of oxygen, in percent by volume, in a flowing oxygen–nitrogen mixture at 23 ± 2 °C that will just support flaming combustion of a specimen under the test conditions. Air contains about 21 % oxygen, so a material with an index well above 21 is harder to keep burning in normal air than one below it.
ISO 4589-2 and ASTM D2863 describe the same procedure for plastics, and the method is also used for cables, insulation, foams and textiles under their own specifications.
How the test works
A small specimen is held vertically in a transparent glass chimney. An oxygen–nitrogen mixture flows upward through the chimney, the top of the specimen is ignited, and the operator watches how long it burns and how far the flame travels. The oxygen concentration is then raised or lowered for the next specimen until the level that just supports burning is found.
Key conditions
In the editions we checked (EN ISO 4589-2:1999 and ASTM D2863-00):
| Condition | Requirement |
|---|---|
| Gas velocity in the chimney | 40 ± 2 mm/s at 23 ± 2 °C |
| Chimney | Heat-resistant glass; at least 450 mm high and 95 mm in diameter preferred (ISO 4589-2) |
| Conditioning | At least 88 h at 23 ± 2 °C and 50 ± 5 % RH, unless otherwise specified |
| Burning criteria | Specimen types I–IV and VI: 180 s of burning or flame reaching 50 mm (top-surface ignition, procedure A). Type V (flexible film in a frame): 180 s or 80 mm below the upper mark on the frame. |
| Sequence | Up-and-down method: lower the oxygen after a specimen exceeds the criterion, raise it after one does not; the final series uses NT − NL = 5. |
Both standards have been revised since these editions, so check the current text before writing a procedure. ISO 4589-2 also includes a short comparison procedure for checking only whether a material is above a stated index.
What LOI does not tell you
Both standards require the report to state that results relate only to the specimens under the test conditions, and must not be used to infer the fire hazard of the material in other forms or other fire conditions. LOI is excellent for ranking formulations and for quality control of a flame-retardant compound. It is not a substitute for a flammability test of the finished product, such as a vertical flame test for a fabric or UL 94 for a plastic part.
Where results go wrong
- Wrong flow. The gas velocity, not just the flow rate, must be right; a different chimney diameter needs a different flow rate.
- Inaccurate oxygen measurement. The index is read directly from the oxygen concentration, so the analyser or mixing system must be calibrated.
- Short conditioning. Moisture changes burning behaviour. Respect the conditioning time.
- Mixing specimen types and ignition procedures. The standards note that different shapes and ignition procedures do not necessarily give equivalent results. Report the form and procedure.
- Drips ignored. Burning drips that descend the specimen count towards the extent of burning.
What the report should contain
Standard and edition · material identification, density and history · specimen form and dimensions · ignition procedure · conditioning · oxygen index to the stated precision · statement that results do not indicate fire hazard in other conditions
Choosing an instrument
The LOI tester has a transparent glass test column and comes in two models: LOI-A01 with automatic control of the oxygen–nitrogen mixture, and LOI-M01 where the operator sets the mixture. It is configured for ISO 4589-2 and ASTM D2863 and suits polymers, cables and insulation, and building materials. For product-level flammability, see our guide which flammability standard applies.
Frequently asked questions
What LOI value means "self-extinguishing"?
No single value does. Air is about 21 % oxygen, so materials with an index above that tend not to keep burning in air under test conditions, but the result only applies to the test geometry. Use the value your specification sets.
Can LOI be used for textiles?
Yes, with a suitable specimen form or support frame and an agreed specification. Report the form used.
Are ISO 4589-2 and ASTM D2863 results comparable?
They describe the same principle and similar conditions, but compare results only when the editions, specimen form and procedure match.