Oxygen transmission rate (OTR) is the volume of oxygen that passes through a flat material per unit area per day, at a stated temperature and humidity. It is usually reported in cm³/(m²·day). It is the number packaging engineers use to compare barrier films for food, pharmaceuticals and other oxygen-sensitive products.
The principle is the same in the common methods. The specimen is clamped as a barrier between two chambers. One side is swept with oxygen, the other with an oxygen-free carrier gas, and a sensor measures how much oxygen arrives on the carrier side. When that amount stops changing, the flow through the film is at steady state and the OTR is calculated over the exposed test area.
Which method
| Method | What it is used for |
|---|---|
| ASTM D3985 | Oxygen transmission through plastic film and sheeting with a coulometric sensor. The reference method for most packaging film specifications. |
| ASTM F1927 | The companion method for testing at controlled relative humidity, for materials whose barrier changes with moisture. |
| ISO 15105-2 | The equal-pressure method of the ISO gas transmission series. ISO 15105-1 is the differential-pressure method, so the part number matters. |
Use the method and edition your customer or specification names. Values from different methods and conditions describe the same film under different circumstances and should not be ranked against each other.
Humidity can change the answer more than the film does
Some of the best oxygen barriers, such as EVOH and polyamide layers, are hygroscopic. As they absorb moisture, their oxygen barrier weakens. A laminate that looks excellent in a dry test can perform very differently at the humidity it meets in use.
That is why the humidity on each side of the specimen is part of the result, not a footnote. If the package will see a humid product or a humid storage room, ask for a test at controlled humidity rather than relying on a dry value.
Temperature matters in the same way. Gas transmission rises with temperature, so an OTR measured at one temperature cannot be used as if it had been measured at another.
Rate, permeance and permeability
- Transmission rate is what the instrument measures for that specimen, in cm³/(m²·day). It includes the effect of thickness.
- Permeance divides the rate by the oxygen partial pressure difference across the film.
- Permeability also multiplies by thickness, so it describes the material rather than the specimen. It is only meaningful for a single, uniform material, not for a multilayer laminate.
Units in older US data are often cm³/(100 in²·day). Because 1 m² is about 15.5 × 100 in², multiply by about 15.5 to convert to cm³/(m²·day), and check that the conditions are the same before comparing.
Where results go wrong
- Leaks at the clamp. Any oxygen that enters around the edge is counted as if it came through the film. Clamp flat specimens without wrinkles, use the specified sealing method, and check the system with an impermeable reference film.
- Creases and pinholes. One fold or puncture in a high-barrier film can dominate the result. Handle specimens flat, and inspect them against light before mounting.
- Stopping too early. High-barrier films can take a long time to reach steady state. Report the value only when the reading has stopped drifting, and record the criterion you used.
- Testing a specimen that does not represent the package. Flat-film OTR does not include seals, folds or closures. It compares materials. It does not predict the shelf life of a finished package on its own.
- Confusing OTR with WVTR. Oxygen and water vapour barriers are separate properties, measured by different methods. A good oxygen barrier is not automatically a good moisture barrier.
What the report should contain
Method and edition · specimen identity, structure and thickness · side facing the oxygen · test temperature · relative humidity on each side · test area · steady-state criterion and test duration · OTR in cm³/(m²·day)
Choosing an instrument
An OTR instrument needs a leak-tight test cell, a defined test area, controlled temperature and, where the method requires it, controlled humidity, plus a sensor sensitive enough for the barrier range you test.
The OTR-01, OTR-02 and OTR-03 have one, two or three test cells with a 50 cm² test area each, a 7-inch touchscreen, and report OTR in cm³/(m²·day) with the test temperature and humidity. They are configured for ASTM D3985, ASTM F1927 and ISO 15105-2. More cells let you test replicates or several materials at the same time. For water vapour barrier, see the WVTR-01A and our article on ASTM E96 wet and dry cup tests.
Frequently asked questions
What is a "good" OTR?
It depends on the product and its shelf life. Lower is a better oxygen barrier, but a value is only meaningful together with its temperature, humidity and method. Agree a target with the packaging specification, not with a general table.
Can I test a whole package?
The methods in this article test flat specimens. Packages need a package-level method and fixture. Flat-film OTR is used to compare and select materials.
Why do two laboratories get different results for the same film?
Most often the conditions differ: humidity, temperature, the side facing the oxygen, or when steady state was declared. Compare the full test conditions before comparing the numbers.